MnZn铁氧体材料特性(BP系列1)

特性
测试条件
符号单位BP40BP44BP47BP90BP90BBP95BP95BBP95QBP95E BP96BP96ABP96BBP96E 
初始磁导率
10KHz
25℃
μi
2300±25%2400±25%2500±25%2200±25%2000±25%3300±25%3300±25%3400±25%3100±25%3300±25%3300±25%3000±25%3000±25%
振幅磁导率
25KHz
200mT
25℃/100℃
μa
450045004500500050005000500038005000500050005300
饱和磁通率
(H=1194A/m)
10KHz
25℃
BsmT510510530540540520540530520530530540520
10KHz
100℃
390390420450460410430420410410425430420
剩磁
25℃BrmT1501201801701709090858480709073
100℃85856085656565706050407055
矫顽力
25℃HcA/m131313131310101210991210
100℃96.566.51166786678.3
功率损耗
100KHz 200mT 正弦波
-40℃PcvkW*m3550400
25℃700600600680750350360300360330280320340
60℃500400400470550300340270290290280300
80℃450350310390
290320260280280260270270
100℃410300250320450300350285310290280280280
120℃500380360460600350380330370350330340320
140℃400380400370
居里温度

Tc>215>215>215>250>275>215>215>215>215>215>215>215>215
电阻率ρ

ρΩ.m6.54446.5664666.5
密度

dkg/m34.84.94.94.94.94.84.854.854.94.94.94.94.9


注:各表格所列之值均用标准环型磁芯所测得的典型值,有特殊要求须在订单或协议中明确提出。